Heat Treated Steel
Chemical Composition
Special CrMoV-alloyed hot work tool steel with excellent high-temperature strength and better
toughness properties than grade 2344 as well as higher thermal conductivity than the classic hot work
tool steels 2343, 2344 and 2367. In comparison to the NiCrMoV – tool steels 2711/2714 HIgh
PERformance DIE is characterized by higher wear resistance, comparable to grade 2343.
Applications
Where there is a requirement for
– Polishability > 400 paper grit
– Sensitive etch designs (e.g. HNO3)
– Higher thermal conductivity
we recommend grade Thruhard Supreme® l
Delivered condition
Annealed to max. 250 HB
Quenched and tempered to customer specifi cation on request to max. 430 HB (approx. 1450 MPa)*
Sizes upon request
Physical properties (reference values)
C | Si | Mn | P | S | Cr | Mo | Ni | V | Others | ||
Typical analysis | 0.35 | 0.35 | 0.50 | 0.025 | 0.003 | 2.70 | 1.00 | 0.60 | 0.20 | + |
Figures in % by mass
CharacteristicsSpecial CrMoV-alloyed hot work tool steel with excellent high-temperature strength and better
toughness properties than grade 2344 as well as higher thermal conductivity than the classic hot work
tool steels 2343, 2344 and 2367. In comparison to the NiCrMoV – tool steels 2711/2714 HIgh
PERformance DIE is characterized by higher wear resistance, comparable to grade 2343.
Applications
- Close-die forging: Small and medium-sized dies and die inserts for a large number of forgings. l
- Highly stressed plastic moulds: Small and medium moulds as well as mould inserts subject to abrasive stress caused by processing of thermosetting plastics, thermoplastics and composite materials also in combination with surface treatments.
Where there is a requirement for
– Polishability > 400 paper grit
– Sensitive etch designs (e.g. HNO3)
– Higher thermal conductivity
we recommend grade Thruhard Supreme® l
- Light alloy processing: Gravity – as well as low pressure die – casting moulds and tools up to 45 HRC.
Delivered condition
Annealed to max. 250 HB
Quenched and tempered to customer specifi cation on request to max. 430 HB (approx. 1450 MPa)*
Sizes upon request
Physical properties (reference values)
Thermal expansion coeffi cient (10–6/K) |
20–100 °C 11.9 |
20–250 °C 12.8 |
20–500 °C 13.8 |
|||
Thermal conductivity (W/mK) |
20 °C 38.3 |
250 °C 37.1 |
500 °C 35.3 |
|||
Young’s modulus (GPa) |
20 °C 209 |
250 °C 204 |
500 °C 198 |